PrusaSlicer 2.9.2 stringing on an Ender 3 S1: retraction settings that worked
Stringing came back when I switched from a generic PLA to a roll of eSUN PLA+ on my Ender 3 S1. Same model I'd printed a dozen times, previously clean, now covered in hair-thin strands between the two towers and across the infill. PrusaSlicer 2.9.2, direct drive, 0.4 mm nozzle.
## It got worse when I raised the temperature
I ran a temperature tower from 220 C down to 195 C in 5 C steps. The strands were worst at 220 and pretty much gone at 205. That told me the filament was being pushed out while the nozzle was travelling, not that retraction distance was magically wrong. So I set nozzle to 205 C and bed to 60 C, then went after the travel settings.
## The retraction values I landed on
These are in Printer Settings > Extruder 1 > Retraction, and they're the ones I'd start with on any direct-drive machine:
retract_length = 0.8
retract_speed = 35
deretract_speed = 25
retract_length_toolchange = 1.2
wipe = 2
travel_speed = 150
The defaults in PrusaSlicer for a stock MK3 are close, but the S1's direct drive needs a shorter pull than a Bowden setup, 0.8 mm instead of the 4-6 mm people were recommending back when everyone had a tube. wipe = 2 matters more than I expected: it wipes the nozzle against the already-printed perimeter during the travel move, which cleans up the little blob that would otherwise become a string.
I also turned on "Avoid crossing perimeters" under Layers & Perimeters. It adds travel distance, but it keeps the long moves over infill instead of across the outside wall.
## What went wrong the first two times
First attempt I set retract_length = 2.4 because that's what a Cura profile I found online used, and I got gaps in the outer wall. The filament didn't have time to re-prime after the long retraction. Looked like under-extrusion and I nearly raised flow to compensate, which would have been the wrong fix.
Second attempt I cranked retraction speed to 60 mm/s. That stripped the filament in the extruder gear after about 20 minutes and the print silently lost extrusion. Turns out my S1's stock extruder doesn't like fast reversals with PLA+.
## The boring check that fixed the last bit
At one point I tried tuning the travel acceleration setting because a forum post claimed it was the culprit. It made no measurable difference and I reverted it. The temperature tower was the only test that actually pointed somewhere useful, so I'd start there next time instead of guessing at numbers one by one.
There were still a few strings on the tallest tower. The cause was a loose hotend fan shroud, the part cooling was blowing sideways onto the nozzle and cooling it unevenly. Tightened two screws. Gone.
I keep a little note taped to the shelf now: 205 C, 0.8 mm, 35 mm/s, wipe 2. If you're on a Bowden machine these numbers will be wrong for you, and if you know a way to auto-tune retraction that doesn't involve printing ten calibration cubes, tell me.